摘要
The cracking characteristics of Alloy 690 in deaerated lwt% NaCl solution with different Na2S2O3 concentrations, namely 0.01, 0.1, 0.2 and 0.5 M, at controlled anodic potentials was investigated by using slow strain rate testing (SSRT) with a strain rate of 1 × 10-6 s-1. The results showed that the ultimate tensile strength and the ductility increased with increasing the concentration of Na2S2O3 at the same anodic potential, but decreased with increasing potential at a fixed concentration of Na2S2O3 Pitting corrosion could occur on Alloy 690 in lwt% NaCl solution with the concentration of Na2S2O3 ≦ 0.1M, depending on the potential. The susceptibilities of Alloy 690 to pitting corrosion and environmentally-assisted cracking in lwt% NaCl solution were inhibited with the concentration of Na2S2O3 ≧ 0.2M, regardless of the potential.
原文 | English |
---|---|
期刊 | NACE - International Corrosion Conference Series |
卷 | 1999-April |
出版狀態 | Published - 4月 1999 |
事件 | Corrosion 1999 - San Antonio, United States 持續時間: 25 4月 1999 → 30 4月 1999 |